| 材料 | ステンレス鋼 | |
|---|---|---|
| Grade | 316L | |
| Main Composition | Fe: bal | |
| Cr: 16~18% | ||
| Ni: 10~14% | ||
| Mo: 2~3% | ||
| Physical Properties | Powder Particle Size | 15-53 μm |
| Flowability (s/50g) | 16~18 | |
| Tap Density (g/cm³) | 4.5~4.7 | |
| Apparent Density (g/cm³) | 4.0~4.2 | |
| Density | Density | 7.9 |
| Sample Theoretical Density | >99% | |
| As-built Properties | Hardness | 13~15HRC |
| Tensile Strength/Rm | 580MPa | |
| Yield Strength/Rp0.2 | 490MPa | |
| Elongation at Break/A | 32% | |
| Reduction of Area/Z | / | |
| Elastic Modulus/E | / | |
| Heat-treated Properties | Hardness | 13~15HRC |
| Tensile Strength/Rm | 670MPa | |
| Yield Strength/Rp0.2 | 550MPa | |
| Elongation at Break/A | 35% | |
| Reduction of Area/Z | 45% | |
| Elastic Modulus/E | 185GPa | |
| 材料 | ステンレス鋼 | |
|---|---|---|
| Grade | 17-4PH | |
| Main Composition | Fe: bal | |
| Cr: 15.5~17.5% | ||
| Ni: 3~5% | ||
| Cu: 3~5% | ||
| Physical Properties | Powder Particle Size | 5-53 μm |
| Flowability (s/50g) | 16~18 | |
| Tap Density (g/cm³) | 4.5~4.7 | |
| Apparent Density (g/cm³) | 4.0~4.2 | |
| Density | Density | 7.9 |
| Sample Theoretical Density | >99% | |
| As-built Properties | Hardness | 18~22HRC |
| Tensile Strength/Rm | 860MPa | |
| Yield Strength/Rp0.2 | 700MPa | |
| Elongation at Break/A | 19% | |
| Reduction of Area/Z | / | |
| Elastic Modulus/E | / | |
| Heat-treated Properties | Hardness | 32~42HRC |
| Tensile Strength/Rm | 1340MPa | |
| Yield Strength/Rp0.2 | 1210MPa | |
| Elongation at Break/A | 13% | |
| Reduction of Area/Z | / | |
| Elastic Modulus/E | / | |
| 材料 | 金型鋼 | |
|---|---|---|
| Grade | 18Ni300 | |
| Main Composition | Fe: bal | |
| Ni: 17~19% | ||
| Co: 8.5~9.5% | ||
| Mo: 4.5~5.2% | ||
| Physical Properties | Powder Particle Size | 15-53 μm |
| Flowability (s/50g) | 19.3 | |
| Tap Density (g/cm³) | 4.8~4.9 | |
| Apparent Density (g/cm³) | 4.2~4.5 | |
| Density | Density | 8.09 |
| Sample Theoretical Density | >99% | |
| As-built Properties | Hardness | 38 ~42 HRC |
| Tensile Strength/Rm | 1177MPa | |
| Yield Strength/Rp0.2 | 980MPa | |
| Elongation at Break/A | 8% | |
| Reduction of Area/Z | 40% | |
| Elastic Modulus/E | 113GPa | |
| Heat-treated Properties | Hardness | 54-57HRC |
| Tensile Strength/Rm | 2163MPa | |
| Yield Strength/Rp0.2 | 1920MPa | |
| Elongation at Break/A | 2.50% | |
| Reduction of Area/Z | 10% | |
| Elastic Modulus/E | 125GPa | |
| 材料 | チタン合金 | |
|---|---|---|
| Grade | TC4 | |
| Main Composition | の: bal | |
| アル: 5.5~6.75% | ||
| V: 3.5~4.5% | ||
| Physical Properties | Powder Particle Size | 15-53 μm |
| Flowability (s/50g) | 36~40 | |
| Tap Density (g/cm³) | 2.7~2.85 | |
| Apparent Density (g/cm³) | 2.3~2.5 | |
| Density | Density | 4.56 |
| Sample Theoretical Density | >99% | |
| As-built Properties | Hardness | 380HV |
| Tensile Strength/Rm | 1000MPa | |
| Yield Strength/Rp0.2 | 950MPa | |
| Elongation at Break/A | 7% | |
| Reduction of Area/Z | / | |
| Elastic Modulus/E | 105GPa | |
| Heat-treated Properties | Hardness | 350HV |
| Tensile Strength/Rm | 1000 | |
| Yield Strength/Rp0.2 | 825 | |
| Elongation at Break/A | 14% | |
| Reduction of Area/Z | / | |
| Elastic Modulus/E | 125GPa | |
| 材料 | アルミニウム合金 | |
|---|---|---|
| Grade | AlSi10Mg | |
| Main Composition | アル: bal | |
| Si: 9.0~11% | ||
| Mg: 0.2~0.45% | ||
| Physical Properties | Powder Particle Size | 15-53 μm |
| Flowability (s/50g) | 150 | |
| Tap Density (g/cm³) | 1.55 | |
| Apparent Density (g/cm³) | 1.3~1.45 | |
| Density | Density | 2.7 |
| Sample Theoretical Density | ≥99.3% | |
| As-built Properties | Hardness | / |
| Tensile Strength/Rm | 420MPa | |
| Yield Strength/Rp0.2 | 240MPa | |
| Elongation at Break/A | 5.50% | |
| Reduction of Area/Z | / | |
| Elastic Modulus/E | 44GPa | |
| Heat-treated Properties | Hardness | / |
| Tensile Strength/Rm | 330MPa | |
| Yield Strength/Rp0.2 | 210MPa | |
| Elongation at Break/A | 11.00% | |
| Reduction of Area/Z | / | |
| Elastic Modulus/E | / | |
| 材料 | アルミニウム合金 (Anodized) | |
|---|---|---|
| Grade | 6061 | |
| Main Composition | アル: bal | |
| Mg: 0.8~1.2% | ||
| Si: 0.4~0.8% | ||
| Physical Properties | Powder Particle Size | 15-53 μm |
| Flowability (s/50g) | 120 | |
| Tap Density (g/cm³) | 1.5 | |
| Apparent Density (g/cm³) | 1.2 | |
| Density | Density | 2.7 |
| Sample Theoretical Density | ≥98% | |
| As-built Properties | Hardness | / |
| Tensile Strength/Rm | 290MPa | |
| Yield Strength/Rp0.2 | 250MPa | |
| Elongation at Break/A | 14% | |
| Reduction of Area/Z | / | |
| Elastic Modulus/E | / | |
| Heat-treated Properties | Hardness | / |
| Tensile Strength/Rm | / | |
| Yield Strength/Rp0.2 | / | |
| Elongation at Break/A | / | |
| Reduction of Area/Z | / | |
| Elastic Modulus/E | / | |
| 材料 | Copper Chromium Zirconium Alloy | |
|---|---|---|
| Grade | CuCrZr | |
| Main Composition | Cu: bal(≥98%) | |
| Cr: 0.5~1.5% | ||
| Zr: 0.05~0.25% | ||
| Physical Properties | Powder Particle Size | 15-53 μm |
| Flowability (s/50g) | 18~22 | |
| Tap Density (g/cm³) | 5.2 | |
| Apparent Density (g/cm³) | 4.0~4.4 | |
| Density | Density | 8.9 |
| Sample Theoretical Density | ≥99.3% | |
| As-built Properties | Hardness | 90HV |
| Tensile Strength/Rm | 350MPa | |
| Yield Strength/Rp0.2 | 250MPa | |
| Elongation at Break/A | 30% | |
| Reduction of Area/Z | / | |
| Elastic Modulus/E | / | |
| Heat-treated Properties | Hardness | 90HV |
| Tensile Strength/Rm | 543MPa | |
| Yield Strength/Rp0.2 | 432 MPa | |
| Elongation at Break/A | 21% | |
| Reduction of Area/Z | / | |
| Elastic Modulus/E | Conductivity IACS: ≥85% | |
| 材料 | Tin Bronze Alloy | |
|---|---|---|
| Grade | CuSn10 | |
| Main Composition | Cu: bal | |
| Sn: 9.0~11% | ||
| Zn: 0.5% | ||
| Physical Properties | Powder Particle Size | 15-53 μm |
| Flowability (s/50g) | 16 | |
| Tap Density (g/cm³) | 5.8 | |
| Apparent Density (g/cm³) | 4.2~4.8 | |
| Density | Density | 8.64 |
| Sample Theoretical Density | ≥98% | |
| As-built Properties | Hardness | 150HV |
| Tensile Strength/Rm | 578MPa | |
| Yield Strength/Rp0.2 | 470MPa | |
| Elongation at Break/A | 23.90% | |
| Reduction of Area/Z | / | |
| Elastic Modulus/E | / | |
| Heat-treated Properties | Hardness | / |
| Tensile Strength/Rm | / | |
| Yield Strength/Rp0.2 | / | |
| Elongation at Break/A | / | |
| Reduction of Area/Z | / | |
| Elastic Modulus/E | / | |
| 材料 | Nickel-based Superalloy | |
|---|---|---|
| Grade | GH4169 | |
| Main Composition | Ni: 50~55% | |
| Cr: 17~21% | ||
| Fe: bal | ||
| Physical Properties | Powder Particle Size | |
| Flowability (s/50g) | 14 | |
| Tap Density (g/cm³) | 4.9 | |
| Apparent Density (g/cm³) | 4.41 | |
| Density | Density | 8.24 |
| Sample Theoretical Density | ≥99% | |
| As-built Properties | Hardness | 220HV |
| Tensile Strength/Rm | 1158MPa | |
| Yield Strength/Rp0.2 | 914MPa | |
| Elongation at Break/A | 14% | |
| Reduction of Area/Z | / | |
| Elastic Modulus/E | / | |
| Heat-treated Properties | Hardness | / |
| Tensile Strength/Rm | / | |
| Yield Strength/Rp0.2 | / | |
| Elongation at Break/A | / | |
| Reduction of Area/Z | / | |
| Elastic Modulus/E | / | |
We own dozens of SLM 3D printers for industrial use.
And the main commonly used metallic materials are these:
- アルミニウム合金 (6061 / AlSi10Mg / 7075)
- ステンレス鋼 (316L / 304L / 17-4 / 347)
- チタン合金 (TC4 / TA1)
- 金型鋼 (S136/HB/CX/1.2709)
- ニッケルリッチ合金 (GH4169 / GH3128 / インコネル625)
- 真鍮合金 (CuCrZr / 錫青銅)
DT is a one – stop 3D printing platform.
Not only because we have dozens of SLM 3D printers and plastic 3D printers, but also, we have invested in 6 3D – printing and CNC machining related factories.

So if you have personalized requirements regarding materials and want to have customized solutions, you can contact us directly.